Quote:
Originally Posted by JT88 View Post
What method do you use with Worcester sauce? Can’t believe I’m asking that 😂
You just paint or splash it on. It's no odder than instant coffee. It's a slow etch and needs renewing as it loses strength, but it does give results, is easily available and does not need special precautions. Rinse off when/if you get the result you want and oil the blade.
David R is offline   Reply With Quote
Old 14th September 2021, 07:07 PM   #2
JT88
Member
 
Join Date: Jun 2021
Posts: 52
Default

Quote:
Originally Posted by David R View Post
You just paint or splash it on. It's no odder than instant coffee. It's a slow etch and needs renewing as it loses strength, but it does give results, is easily available and does not need special precautions. Rinse off when/if you get the result you want and oil the blade.
What kind of timeline are you talking about for the application? May give it a try.
JT88 is offline   Reply With Quote
Old 15th September 2021, 01:47 AM   #3
A. G. Maisey
Member
 
Join Date: May 2006
Posts: 6,992
Default

I'm not going to say anything about wootz, I do not understand the material, and I do not know how to recognise the types nor how to etch & stain them.

But I do understand mechanical damascus and Malay World pamor. I have made quite a lot of both, and cleaned, etched and stained quite a lot of both, and I have been doing this with both recently made & historic material for a very long time.

The damascus I have made myself I have usually stained with ferric chloride, just the pre-prepared mix that is used for etching circuit boards. Yes, it can be difficult to achieve a satisfactory result with it. I apply with an old soft toothbrush, over the laundry tub, with the cold water tap running. I rinse off, dry, and reapply until I get the colour I want, then I paint on a slurry of bicarb of soda, let it sit for a few minutes, thoroughly rinse, dry with a lint free cloth, then a hairdryer. Spray with WD40.

On damascus I have used various other acidic solutions, but overall I have achieved the best results with ferric chloride.

On historic mechanical damascus, and on pamor --- which is essentially mechanical damascus sometimes with a nickel content --- I usually use laboratory quality white arsenic mixed as a paste with fresh Tahitian lime juice.

Let me be very clear:- I do not recommend that anybody without proper training and permits attempt to play with any kind of arsenic.

On just about any ferric material I am a big fan of white household vinegar. It cleans things beautifully and on some materials it will impart some degree of stain.
A. G. Maisey is offline   Reply With Quote
Reply

Thread Tools Search this Thread
Search this Thread:

Advanced Search
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off

Forum Jump


All times are GMT +1. The time now is 05:44 AM.


Powered by vBulletin® Version 3.8.11
Copyright ©2000 - 2025, vBulletin Solutions Inc.
Posts are regarded as being copyrighted by their authors and the act of posting material is deemed to be a granting of an irrevocable nonexclusive license for display here.